耐候用热轧带钢
- 
        
累计评价0  - :耐候用热轧带钢
 
                                                                                                 
                                                                                     | 
                
产品用途
该系列产品主要用于制造于铁路车辆、火车车厢和塔架等,具有较高的强度和优良的耐大气腐蚀性能,适合焊接加工和冷弯成型等。
供货牌号及标准
牌号  | 标准  | 用途  | 备注  | 
Q450NQR1  | 
 TB/T 1979  | 
 铁路用  | Q500NQR1: Re≥500MPa,1 表示 Cu、Cr、Ni 类  | 
Q500NQR1  | |||
Q550NQR1  | |||
09CuPCrNi-A  | 
 TB/T 1979  | 
 铁路用  | 
 -  | 
09CuPCrNi-B  | |||
SPA-H  | JIS G3125  | 集装箱用  | -  | 
Q235NH  | 
 
 
 
 GB/T4171  | 
 
 
 车辆、桥梁、集装箱、建筑、塔架等  | 
 
 
 
 -  | 
Q295NH  | |||
Q355NH  | |||
Q415NH  | |||
Q460NH  | |||
Q500NH  | |||
Q550NH  | 
化学成分
 牌号  | 化学成分(%)  | |||||||
C  | Si  | Mn  | P  | S  | Cr  | Cu  | Ni  | |
Q450NQR1  | ≤0.10  | ≤0.70  | ≤1.50  | ≤0.020  | ≤0.006  | 0.30~1.25  | 0.20~0.55  | 0.12~0.65  | 
Q500NQR1  | ≤0.10  | ≤0.70  | ≤2.00  | ≤0.020  | ≤0.006  | 0.30~1.25  | 0.20~0.55  | 0.12~0.65  | 
Q550NQR1  | ≤0.14  | ≤0.70  | ≤2.00  | ≤0.020  | ≤0.006  | 0.30~1.25  | 0.20~0.55  | 0.12~0.65  | 
09CuPCrNi-A  | ≤0.12  | 0.25~0.75  | 0.20~0.50  | 0.06~0.12  | ≤0.020  | 0.30~1.25  | 0.25~0.50  | 0.12~0.65  | 
09CuPCrNi-B  | ≤0.12  | 0.10~0.40  | 0.20~0.50  | 0.06~0.12  | ≤0.020  | 0.30~0.65  | 0.25~0.45  | 0.25~0.50  | 
SPA-H  | ≤0.12  | 0.25~0.75  | ≤0.60  | 0.07~0.15  | ≤0.035  | 0.30~1.25  | 0.25~0.55  | 0.12~0.65  | 
Q235NH  | ≤0.13  | 0.10~0.40  | 0.20~0.60  | ≤0.030  | ≤0.030  | 0.40~0.80  | 0.25~0.55  | ≤0.65  | 
Q295NH  | ≤0.15  | 0.10~0.50  | 0.30~1.00  | ≤0.030  | ≤0.030  | 0.40~0.80  | 0.25~0.55  | ≤0.65  | 
Q355NH  | ≤0.16  | ≤0.50  | 0.50~1.50  | ≤0.025  | ≤0.030  | 0.40~0.80  | 0.25~0.55  | ≤0.65  | 
Q415NH  | ≤0.12  | ≤0.65  | ≤1.10  | ≤0.025  | ≤0.030  | 0.30~1.25  | 0.20~0.55  | 0.12~0.65  | 
Q460NH  | ≤0.12  | ≤0.65  | ≤1.50  | ≤0.025  | ≤0.030  | 0.30~1.25  | 0.20~0.55  | 0.12~0.65  | 
Q500NH  | ≤0.12  | ≤0.65  | ≤2.00  | ≤0.025  | ≤0.030  | 0.30~1.25  | 0.20~0.55  | 0.25~0.50  | 
Q550NH  | ≤0.16  | ≤0.65  | ≤2.00  | ≤0.025  | ≤0.030  | 0.30~1.25  | 0.20~0.55  | 0.12~0.65  | 
 
力学性能
 牌号  | 拉伸试验  | 
 180°弯曲试验弯心直径  | |||
屈服强度 Re(MPa)  | 抗拉强度 Rm(MPa)  | 
 延伸率A(%)  | 屈强比 Re/Rm  | ||
Q450NQR1  | ≥460  | ≥550  | ≥22  | 
 
 
 ≤0.75  | 
 
 D=a (H≤6mm) D=2a(H>6mm)  | 
Q500NQR1  | ≥510  | ≥600  | ≥18  | ||
Q550NQR1  | ≥560  | ≥600  | ≥18  | ||
09CuPCrNi-A  | ≥345  | ≥480  | ≥24  | ||
09CuPCrNi-B  | ≥295  | ≥431  | ≥24  | ||
SPA-H  | ≥355  | ≥490  | ≥22  | -  | -  | 
Q235NH  | ≥235  | 360~510  | ≥25  | -  | -  | 
Q295NH  | ≥295  | 430~560  | ≥24  | -  | 
 
 D=a (H≤6mm) D=2a(H>6~16) D=3a (H>16mm)  | 
Q355NH  | ≥355  | 490~630  | ≥22  | -  | |
Q415NH  | ≥415  | 520~680  | ≥22  | -  | |
Q460NH  | ≥460  | 570~730  | ≥20  | -  | |
Q500NH  | ≥500  | 600~760  | ≥18  | -  | |
Q550NH  | ≥550  | 620~780  | ≥16  | -  | |

                                                                                    